Materials & grades
1070 high-carbon steel: equivalents 070A72 (EN42), 70C6, C67S and S70C
1070 is a high-carbon steel with about 0.70 % carbon, used for springs, spring wire, blades and wear parts after hardening and tempering. Its closest equivalents are 070A72 (old EN42) in the UK, 70C6 in India, C67S and C75S (1.1231, 1.1248) in Europe, and S70C or SWRH72A in Japan.
Names by standard
What it is called in each region
| Region | System | Designation | 規格 | Match |
|---|---|---|---|---|
| USA | AISI/SAE | 1070Composition limits shown are SAE J403 (P ≤0.030 %). ASTM A29 and older AISI tables give P ≤0.040 %. | SAE J403; ASTM A510 / A576 (10L70) / A713 (wire) / A830 | Same material |
| UNS | G10700 | — | Same material | |
| UK | BS 970 | 070A72Carbon 0.70–0.75 %, manganese 0.60–0.80 %: a narrower carbon range than 1070 (Total Materia). | BS 970-1 | Closest equivalent |
| BS 970 (1955 EN series) | EN42Superseded 1955 name. Roymech ties EN42 to 070A72; Total Materia also uses it for 070A78. | — | Closest equivalent | |
| BS 1449 / BS 5770 | CS70Cold-rolled spring strip with carbon 0.65–0.75 %, matching 1070's carbon range (West Yorkshire Steel). | BS 5770-2 (withdrawn) | Closest equivalent | |
| EU | EN 10027-1 name | C67S (1.1231)Cold-rolled strip for springs. Carbon 0.65–0.73 %, with tighter phosphorus and sulphur than 1070. | EN 10132-4 | Closest equivalent |
| EN 10027-1 name | C75S (1.1248)Cold-rolled strip for springs. Carbon 0.70–0.80 %, the next step up from C67S. | EN 10132-4 | Closest equivalent | |
| EN 10027-1 name | C70D (1.0615)Wire-rod grade listed against 070A72 by Total Materia. Composition limits not tabulated here. | EN 10016 / EN ISO 16120 (wire rod) | Closest equivalent | |
| DIN (legacy) | Ck67 / Ck75Superseded German names for C67S and C75S. | — | Closest equivalent | |
| インド | IS 1570 | 70C6Carbon 0.65–0.75 %, the same as 1070, with manganese 0.50–0.80 %. | IS 1570 (Part 2/Sec 1) | Closest equivalent |
| IS 1570 (old designation) | C70Superseded Indian name for 70C6. | — | Closest equivalent | |
| Japan | JIS G 4051 | S70CCarbon 0.65–0.75 % and manganese 0.60–0.90 %, the same limits as 1070, but offered only as plates, sheets and strips. | JIS G 4051 (Annex JB) | Equivalent |
| JIS G 4802 | S70C-CSPCold-reduced spring strip with carbon 0.65–0.75 %. | JIS G 4802 | Closest equivalent | |
| JIS G 3506 | SWRH72A / SWRH72BHigh-carbon wire rod for drawing, with carbon 0.69–0.76 % (manganese 0.30–0.60 % for A, 0.60–0.90 % for B). | JIS G 3506 | Closest equivalent |
On equivalence
- No single European grade matches 1070 exactly. EN ISO 683-1 stops at C60, so the nearest are the EN 10132-4 strip grades C67S (0.65–0.73 % C) and C75S (0.70–0.80 % C), each with tighter phosphorus and sulphur and a silicon requirement that 1070 does not have.
- Do not use the designation C70 for 1070 steel. The material number 1.1520, which some cross-reference lists attach to C70, belongs to a tool steel in a different standard.
- Sources disagree on EN42. Roymech ties it to 070A72 and Total Materia lists it against 070A78 too, so treat the old EN42 name as covering the 0.70–0.80 % carbon spring range rather than one exact code.
- In Japan, S70C is in JIS G 4051 only for plates, sheets and strips. For round bar the usual route is the SWRH wire-rod grades or a spring-strip grade in JIS G 4802.
- Indian 70C6 has the same carbon range as 1070 but lower manganese (0.50–0.80 % against 0.60–0.90 %). IS 1570 fixes only carbon and manganese.
Chemical composition
Composition limits, mass %
| Element | 1070USA · SAE J403 | 070A72UK · BS 970-1 (composition as cited from BS 1429:1980) | CS70UK · BS 1449 / BS 5770 | C67S (1.1231)EU · EN 10132-4 | C75S (1.1248)EU · EN 10132-4 | 70C6インド · IS 1570 (Part 2/Sec 1):1979 | S70CJapan · JIS G 4051 (Annex JB) | SWRH72AJapan · JIS G 3506:2024 |
|---|---|---|---|---|---|---|---|---|
| C | 0.65–0.75 | 0.70–0.75 | 0.65–0.75 | 0.65–0.73 | 0.70–0.80 | 0.65–0.75 | 0.65–0.75 | 0.69–0.76 |
| Si | — | — | 0.05–0.35 | 0.15–0.35 | 0.15–0.35 | — | 0.15–0.35 | — |
| Mn | 0.60–0.90 | 0.60–0.80 | 0.50–0.90 | 0.60–0.90 | 0.60–0.90 | 0.50–0.80 | 0.60–0.90 | 0.30–0.60 |
| P | ≤0.030 | ≤0.050 | ≤0.045 | ≤0.025 | ≤0.025 | — | ≤0.030 | ≤0.030 |
| S | ≤0.050 | — | ≤0.045 | ≤0.025 | ≤0.025 | — | ≤0.035 | — |
| Cr | — | — | — | ≤0.40 | ≤0.40 | — | ≤0.20 | — |
| Ni | — | — | — | ≤0.40 | ≤0.40 | — | ≤0.20 | — |
| Mo | — | — | — | ≤0.10 | ≤0.10 | — | — | — |
| Cu | — | — | — | — | — | — | ≤0.30 | — |
| Cr+Ni | — | — | — | — | — | — | ≤0.35 | — |
Mechanical properties
Strength and hardness
| Condition | Tensile strength | Yield strength | Elongation | Hardness |
|---|---|---|---|---|
| Hot-rolled bar, estimated minimum (1070)Estimated minimum, SAE J1397 basis; typical values run higher and section size is not statedSAE J1397 estimated minimum values as published by ICAST; typical values run higher and section size is not stated | 700 MPa102 ksi | 390 MPa57 ksi | 12 % | — |
| Annealed and skin passed strip (C67S)Specified maximum, EN 10132-4EN 10132-4 as tabulated by Roymech | ≤640 MPa≤93 ksi | ≤510 MPa≤74 ksi | ≥16 % | ≤200 HV |
| Quenched and tempered strip (C67S / C75S)Specified range, EN 10132-4EN 10132-4 as tabulated by Roymech | 1200–1900 MPa174–276 ksi | — | — | 370–580 HV |
In practice
Behaviour, heat treatment and uses
Characteristics
- About 0.70 % carbon gives high strength, hardness and spring temper with low ductility; SAE J1397 estimates only about 12 % elongation as hot rolled.
- Hardenable by oil or water quench and tempered to the strength required; plain carbon steels have low hardenability, so only thin sections harden through.
- Common in strip and wire form: EN 10132-4 strip grades C67S and C75S are specified for springs, and ASTM A713 lists 1070 for wire.
- Welding is not normally recommended at this carbon level; heating for welding needs preheat and stress relief and the heat-affected zone is brittle.
- Matthey notes its C75E strip is less ductile than C60E strip, which shows the trend as carbon rises.
Heat treatment
- Normalizing: about 900 °C (1650 °F) for C75E strip (Matthey), cooled in air.
- Soft annealing: about 650–720 °C (1200–1330 °F) for C75E strip (Matthey).
- Hardening: about 820–850 °C (1510–1560 °F) with an oil quench for 070A72 (Total Materia); 790–820 °C (1455–1510 °F) in water or oil for C75E strip (Matthey).
- Tempering: depends on the hardness required; Matthey gives 350–700 °C (660–1290 °F) for C75E strip.
- Spring stress relief after coiling: 385–399 °C (725–750 °F), held at least 1 hour, then air cooled (Total Materia, SAE 1070).
主な用途
- Flat springs, clutch plates and shims
- Hardened and tempered blades, saw blades and doctor blades
- Agricultural and masonry tools
- Drawn spring wire and wire products
Carbon steels
Similar grades compared
| グレード | C % | Mn % | Cr % | Ni % | Tensile, first listed condition |
|---|---|---|---|---|---|
| 1070 / 070A72 | 0.65–0.75 | 0.60–0.90 | ≤0.40 | ≤0.40 | 700 MPa |
| 1060 / C60 | 0.55–0.65 | 0.60–0.90 | ≤0.40 | ≤0.40 | 680 MPa |
| 1080 / 80C6 | 0.75–0.88 | 0.60–0.90 | ≤0.30 | ≤0.40 | 700 MPa |
| 1095 / C100S | 0.90–1.03 | 0.30–0.50 | ≤0.40 | ≤0.40 | 830 MPa |
| 1008 | ≤0.10 | 0.30–0.50 | — | — | 303 MPa |
| 1010 / C10E | 0.08–0.13 | 0.30–0.60 | ≤0.30 | — | 320 MPa |
| 1015 / C15E | 0.13–0.18 | 0.30–0.60 | ≤0.30 | — | 340 MPa |
| 1018 | 0.15–0.20 | 0.60–0.90 | ≤0.20 | — | 400 MPa |
| 1020 / C22E | 0.18–0.23 | 0.30–0.60 | ≤0.30 | ≤0.40 | 380 MPa |
| 1025 / C25E | 0.22–0.28 | 0.30–0.60 | ≤0.30 | ≤0.40 | 400 MPa |
Composition from the US standard where one exists, otherwise the first standard listed on each grade's page. Strength conditions differ between grades; open a grade for its full table.
よくあるご質問
Common questions
What is the equivalent of 1070 steel?
070A72 (old EN42) in the UK, 70C6 in India and S70C or SWRH72A in Japan are the usual equivalents. In Europe the nearest are the spring-strip grades C67S (1.1231) and C75S (1.1248). None is identical to 1070.
Is 1070 a spring steel?
Yes. Its 0.65–0.75 % carbon and hardenability suit springs, spring strip and spring wire, and ASTM A713 and EN 10132-4 list grades in this range. It is lower in cost than alloy spring steels but has lower hardenability.
What is the difference between 1070 and 1080?
1080 has more carbon (0.75–0.88 % against 0.65–0.75 %), so it hardens harder and is less ductile. Manganese is the same, 0.60–0.90 %. Both have low hardenability.
Is 1070 weldable?
Not readily. At 0.65–0.75 % carbon the heat-affected zone becomes hard and brittle. Welding needs preheat and post-weld heat treatment, and it is usually avoided.
What is the Japanese equivalent of 1070?
SWRH72A or SWRH72B wire rod (JIS G 3506, 0.69–0.76 % carbon) and S70C-CSP spring strip (JIS G 4802) are used. S70C in JIS G 4051 has the same limits as 1070 but only for plates, sheets and strips.
From the Corona catalog
Need a part made to this specification?
Send the drawing, the material or grade, the finish, the quantity and the delivery country. The team reviews the requirement and the manufacturing route.
お問い合わせを始めるKeep reading
Related references
References
Sources
- SAE J403: Chemical Compositions of SAE Carbon Steels — Governs the US composition limits for 1060, 1070, 1080 and 1095.
- ICAST: SAE J403 / SAE J1397 UNS G10700, Hot Rolled — J1397 estimated minimum properties.
- Roymech: EN 10132 cold rolled narrow steel strip for heat treatment — EN 10132-4 spring-steel grades C60S to C100S: composition and strip properties.
- JIS G 4051: Carbon steels for machine structural use (Japanese Standards Association) — Limits for S58C, S60C, S65C, S70C and S75C checked against the 2016 edition; S60C to S75C apply only to plates, sheets and strips (Annex JB).
- IS 1570 (Part 2/Sec 1):1979 Schedules for wrought steels: carbon steels (public copy) — Table 1 carbon and manganese limits; Table 2 hot-rolled or normalized tensile limits.
- Total Materia: SAE 1070 — SAE J403:2014 composition and spring stress-relief treatment.
- Total Materia: B.S. 070 A 72 — Composition, heat treatment and cross-references; lists En42.
- Lamineries Matthey: Ck75 (C75E) strip datasheet — Heat treatment temperatures for C75E strip.
- Roymech: British Standard steel numbers — Links old EN numbers to BS 970 codes: 43D with 080A62, 42 with 070A72, 44 with 060A96.
- Total Materia: JIS S70C-CSP (JIS G 4802) — Carbon 0.65–0.75 %.
- Total Materia: JIS SWRH72A (JIS G 3506:2024) — Carbon, manganese and phosphorus limits.
- West Yorkshire Steel: CS70 spring steel — CS70 composition and related BS 1449 / BS 5770 names.
- BS 5770-2: steel strip for springs, cold rolled carbon and low alloy (withdrawn 2000) — Superseded British strip specification behind the CS70 to CS100 names.
- Nippon Steel: special steel sheet and strip catalogue (U006) — Mill check of S70C composition (strip grade).
- Tata Steel Thailand: high carbon wire rod grades (JIS G 3506) — SWRH62A/B, 72A/B and 82A/B carbon, silicon, manganese, phosphorus and sulphur.
- Rewon: BS 970 carbon steel grades with nearest SAE — Independent check of the BS 970 A-series carbon and manganese limits and the 080A62 / En43D pairing.
Values summarize published limits and typical data. The governing standard and the current edition control; check them before specifying.